What ASTM A572 Grade 42 Is
ASTM A572/A572M is the specification for high-strength low-alloy structural steel, covering plates, shapes, sheet piling and bars in a series of strength grades. Grade 42 is the entry grade of that series, defined by a minimum yield strength of 42 ksi, or about 290 MPa. The strength comes from small microalloying additions of niobium or vanadium rather than from a high carbon level, so the grade remains weldable and formable in ordinary structural shops, unlike the older high-carbon structural steels it replaced. When the material is needed in tubular form, the pipe is ordered against a pipe specification with the A572 chemistry and property requirements quoted in the purchase order; the grade marking, heat number and test results then travel with the material and form the basis of the inspection record on site.
Grade 42 has never been a pressure-pipe grade. It is selected on the basis of stiffness and strength of a structure, and any application involving internal pressure must be reviewed against a pressure pipe specification instead.
Chemical Composition and Mechanical Properties
| Item | Requirement for Grade 42 |
|---|---|
| Carbon | 0.21 % max |
| Manganese | 1.35 % max |
| Phosphorus | 0.04 % max |
| Sulfur | 0.05 % max |
| Silicon | 0.40 % max |
| Microalloying | Niobium 0.005 – 0.05 % or vanadium 0.01 – 0.15 %, added singly or in combination |
| Yield strength | 290 MPa (42 ksi) min |
| Tensile strength | 415 MPa (60 ksi) min |
| Elongation | 20 % min on a 200 mm gauge length for the thicknesses in common structural use |
The tabulated minimum elongation falls as section thickness rises, and the specification applies its own rules for the tension test location and orientation, so the value printed on a mill certificate should always be read together with the thickness and the test direction. Impact testing is not a routine requirement of the grade; where toughness at a stated temperature matters, a Charpy V-notch requirement with a specific test temperature and energy level must be written into the order, and that requirement should name the temperature the structure will actually experience. Hardness in the normalized or as-rolled condition normally falls in the range of roughly 130 to 180 HB.
Where Grade 42 Pipe and Tube Are Used
Building frames, mezzanine structures and industrial plant supports where a modest strength increase over carbon steel reduces steel weight.
Bridge and highway structures of moderate span, and secondary bridge members such as bracing and stiffeners.
Transmission and communication towers, lighting masts and monopole structures.
Pipe racks, conveyor gantries, crane runways and equipment skids in industrial plants.
Boom sections and structural members of mobile cranes and lifting equipment, where the strength-to-weight ratio governs capacity.
Fabrication and Welding Practice
The low carbon and microalloyed chemistry allow welding with ordinary low-hydrogen procedures. For shielded metal arc work use an E70 class electrode, and for gas-shielded work an ER70S class wire matched to the base metal strength. Sections up to about 25 mm thick can usually be welded without preheat in normal shop conditions, but thick sections, high restraint joints and low ambient temperatures call for preheat in the range of 100 to 150 °C, with the exact value fixed by a qualified welding procedure. Keep heat input within the range qualified for the consumable: excessive heat input coarsens the heat-affected zone, while very low heat input with a high-strength consumable can produce hard, crack-prone zones.
For cold forming, respect a minimum bend radius that reflects the thickness of the section; a radius of about twice the section depth or pipe diameter is a common shop starting point, and tighter bends should be qualified by a test piece because the microalloyed grade work-hardens quickly. Hot-dip galvanizing or a protective coating system is required for outdoor exposure, and venting and draining holes must be designed into closed tubular assemblies before galvanizing.
Purchasing and Inspection Checkpoints
Confirm on the certificate that the grade is stated as Grade 42 and that the niobium or vanadium addition is reported, since a heat without the microalloying addition cannot be expected to meet the yield strength. Check the yield and tensile results together with the elongation value and the test location, verify the heat number against the physical marking on the pipe, and review the thickness and dimensional tolerances against the drawing before fabrication starts. Where the structure will be welded under a qualified procedure, obtain the material certificate early enough to run the procedure qualification with the actual grade, and keep a sample of the delivered heat for that purpose.
FAQ
Q: What does the 42 in ASTM A572 Grade 42 mean?
It refers to the minimum yield strength of 42 ksi, which is about 290 MPa. The grade number in this specification is a strength indicator, not a chemistry code.
Q: Is Grade 42 stronger than ordinary structural carbon steel?
Yes. Its minimum yield strength of 290 MPa is roughly 15 % above that of common structural carbon steel at 250 MPa, which is why the same load can often be carried with a lighter section.
Q: Can Grade 42 be used for pressure piping?
It is a structural steel specification, not a pressure pipe specification. For pressure service the pipe should be ordered to a pressure pipe standard with the appropriate test requirements.
Q: Does Grade 42 need preheating before welding?
Thin and medium sections welded with a qualified low-hydrogen procedure generally need no preheat. Thick sections, high restraint joints and cold weather conditions call for preheat in the 100 to 150 °C range, confirmed by the qualified procedure.
Q: How should the order be written?
State the grade, the product form and dimensions, the chemistry and property requirements of the specification, the tolerance class, and any supplementary requirement such as impact testing or a certificate of compliance.
Q: What documents should accompany the delivery?
A mill test certificate showing heat number, chemistry, tensile and yield results, elongation and any supplementary test results, together with the marking on each piece or bundle.