Welding technology of Q345D steel pipe


Q1: How to determine the preheating temperature when welding Q345D steel pipe?
The preheating temperature is mainly determined by the wall thickness of the steel pipe: when the wall thickness is ≤20mm, the preheating temperature is ≥80℃; when the wall thickness is 20-40mm, the preheating temperature is 100-120℃; when the wall thickness is >40mm, the preheating temperature is ≥150℃. When the ambient temperature is lower than 0℃, it is necessary to increase the calculated value by 20℃. The preheating range should cover an area of 3 times the plate thickness on both sides of the weld, and should not be less than 100mm. Use an infrared thermometer to monitor the groove and surrounding temperature in real time to ensure uniform heating. The interlayer temperature must be strictly controlled below 250℃ to avoid deterioration of the microstructure and performance in the overheating zone.

Q2: What welding materials are recommended for welding Q345D steel pipes?
For manual arc welding, CHE507DR welding rod (-40℃ impact energy ≥47J) is recommended, which needs to be dried at 350℃×1h before use. Submerged arc welding should use SJ101 flux with S2Ni welding wire (containing 1.5% nickel) to improve the low-temperature toughness of the weld. ER80S-G welding wire (80%Ar+20%CO₂ shielding gas) is recommended for gas shielded welding. The water content of all fluxes must be ≤0.10%, and the sulfur content of welding wire must be ≤0.008%. For important structures, the weld metal properties must be retested to ensure that they meet the design requirements.

Q3: How to prevent cold cracks in Q345D steel pipe welding?
The diffusible hydrogen content must be strictly controlled (glycerol method detection ≤5ml/100g), and low-hydrogen welding materials must be selected. Strictly implement preheating and interlayer temperature control requirements to ensure that the welding area maintains an appropriate temperature. Post-heat treatment (250-300℃×1h) is performed immediately after welding to promote hydrogen escape. For joints with large restraint, the low-strength matching principle is adopted (the strength of the welding material is one level lower than that of the parent material). 100% magnetic particle testing (MT) must be carried out 24 hours after welding to check for surface cracks.

Q4: What are the key points to pay attention to when welding Q345D with dissimilar stainless steel?
The transition layer must use nickel-based welding materials (such as ENiCrMo-3) with a thickness of ≥4mm to block carbon migration. Strictly control the heat input ≤15kJ/cm to avoid embrittlement of the fusion zone. The Q345D side groove angle is increased to 70° to reduce the dilution rate on the stainless steel side. Slow cooling measures are taken after welding to prevent the formation of hardened structures due to rapid cooling. After the RT test is qualified, the fusion line must also be tested for microhardness (required to be ≤350HV10).

Q5: What are the special requirements for the welding process assessment of Q345D steel pipes?
The impact specimen must include three locations: the center of the weld, the fusion line, and the heat-affected zone (fusion line + 2mm). The test temperature must be 20℃ lower than the design temperature (if the design is -20℃, do a -40℃ impact). The bending test shall preferably use side bending specimens (when the wall thickness is ≤38mm). The hardness test shall cover the weld, heat-affected zone and parent material (required to be ≤248HV10). The process assessment shall cover all welding positions (especially the 6G position) to ensure the reliability of welding in all positions.