What Is S235JR (1.0037)?
S235JR is a non-alloy structural steel grade defined in EN 10025-2, with material number 1.0037. The designation reads as follows: S stands for structural steel, 235 is the minimum yield strength of 235 MPa at a thickness of 16 mm or less, and JR means the grade requires a minimum Charpy V-notch impact energy of 27 J at room temperature, plus 20 deg C. The material is supplied as plates, sections, bars, and strip for welded pipe production, and it is one of the most frequently specified carbon steels in European construction and mechanical engineering.
Chemical Composition per EN 10025-2
Typical cast analysis limits for S235JR: carbon 0.17 percent max for thickness up to 40 mm and 0.20 percent max above 40 mm; manganese 1.40 percent max; phosphorus 0.025 percent max; sulfur 0.025 percent max; nitrogen 0.012 percent max; copper 0.55 percent max when specified. The low carbon content keeps the steel readily weldable in most sections without preheat, which is one of the main reasons it dominates general fabrication work.
Mechanical Properties
Minimum yield strength (ReH): 235 MPa for thickness up to 16 mm, 225 MPa for 16 to 40 mm, 215 MPa for 40 to 63 mm, and 205 MPa for 63 to 80 mm. Tensile strength Rm is 360 to 510 MPa for thickness up to 100 mm. Minimum elongation A is 26 percent for thickness up to 40 mm and 24 percent for 40 to 100 mm. Charpy V-notch impact energy is 27 J minimum at plus 20 deg C. For comparison, the J0 variant requires 27 J at 0 deg C and J2 requires 27 J at minus 20 deg C; choose these variants when the structure is exposed to lower service temperatures.
Global Equivalents
Common functional equivalents include: ASTM A36 (USA), which specifies 250 MPa minimum yield and 400 to 550 MPa tensile strength; JIS G3101 SS400 (Japan), 245 MPa minimum yield and 400 to 510 MPa tensile strength; GB/T 700 Q235B (China), 235 MPa minimum yield and 370 to 500 MPa tensile strength; and the retired German designation St37-2. These grades are similar in strength class but are not identical in chemical composition, impact testing, or certification requirements, so substitution must always be confirmed against the project specification and applicable building code.
Machinability and Weldability
S235JR machines well with standard tooling because of its low carbon content and moderate hardness. Cutting, drilling, milling, and turning can be performed with conventional speeds and feeds; softness occasionally produces built-up edge or burring, which is controlled with sharp tools, suitable cutting fluids, and optimized parameters. Weldability is excellent across all common processes: shielded metal arc, gas metal arc, flux cored, submerged arc, and resistance welding are all used on this grade. For structural fabrication, execution and inspection follow the requirements of EN 1090-2.
Typical Applications
S235JR is used for building frames and secondary structures, platforms, stairs, handrails, agricultural equipment, machine frames, low-pressure conveying systems, tanks, and general fabrication. It is also a common raw material for welded steel pipe in structural and low-pressure fluid service, where the combination of formability, weldability, and predictable strength keeps fabrication cost low.
Frequently Asked Questions
What does the number 1.0037 mean? It is the material number (Werkstoffnummer) assigned to S235JR in the European steel numbering system, used on mill certificates and in specifications to identify the grade unambiguously.
Is ASTM A36 the same as S235JR? Not exactly. A36 specifies 250 MPa minimum yield and 400 to 550 MPa tensile, with looser limits on carbon, phosphorus, and sulfur. S235JR specifies 235 MPa yield, 360 to 510 MPa tensile, and stricter composition limits. They are functionally similar for many structural jobs but not interchangeable without checking the specification.
What is the difference between S235JR and S235J2? Both have the same strength; the suffix defines impact testing temperature. JR is tested at plus 20 deg C, J0 at 0 deg C, and J2 at minus 20 deg C, all with 27 J minimum average energy. J2 is preferred for outdoor structures in cold climates.
Can S235JR be welded without preheat? In most sections up to about 30 mm and under controlled shop conditions, preheat is not required. For thicker sections, cold forming, or restrained joints, apply a light preheat of 50 to 100 deg C and use low-hydrogen consumables.
What is the yield strength of S235JR at 50 mm thickness? The minimum yield strength drops to 215 MPa for thickness between 40 and 63 mm, so design calculations must use the value that matches the actual section thickness.