Jun 04, 2025 Leave a message

ASTM A335 Grades Explained: P5, P9, P11, P22, P91 and P92 Alloy Steel Pipe

What Is ASTM A335 Pipe?

ASTM A335 is the standard specification for seamless ferritic alloy-steel pipe for high-temperature service. The grades covered by the specification are chromium-molybdenum steels that keep their strength and resist oxidation and creep at elevated temperature, which is why they are the default choice for main steam, hot reheat and high-temperature process lines in power stations, refineries and petrochemical plants. Every length supplied to ASTM A335 is seamless, and the pipe is ordered by grade designator such as P5, P11, P22 or P91 together with nominal diameter, wall thickness and length.

Grade Range and Chromium Content

The grades are written as the letter P followed by a number that broadly reflects chromium and molybdenum content:

P5, P5b and P5c: nominal 4 to 6% Cr with about 0.5% Mo, used where oxidation resistance is required

P9: nominal 9% Cr with about 1% Mo

P11, P11b, P12, P12b and P15: 1.00 to 1.50% Cr or 1% Cr types for moderate elevated-temperature duty

P21, P22 and P22b: nominal 2.25% Cr with about 1% Mo, the most widely used refinery and boiler grade

P91, P911 and P92: 9% Cr martensitic grades with vanadium and niobium additions for advanced high-temperature service

Chromium raises oxidation resistance, while molybdenum provides solid-solution strengthening and improves creep behaviour. The 9% Cr grades also contain controlled vanadium, niobium and nitrogen and are supplied in the normalised and tempered condition instead of the fully annealed condition used for the lower grades.

Chemical and Mechanical Requirements

The specification controls heat analysis and product analysis for each grade, and requires tensile testing of the finished pipe. Nominal compositions and minimum room-temperature properties are summarised below.

Grade Nominal Cr Nominal Mo Min tensile strength Min yield strength
P5 4.00-6.00% 0.45-0.65% 415 MPa (60 ksi) 205 MPa (30 ksi)
P9 8.00-10.00% 0.90-1.10% 415 MPa (60 ksi) 205 MPa (30 ksi)
P11 1.00-1.50% 0.44-0.65% 415 MPa (60 ksi) 205 MPa (30 ksi)
P12 0.80-1.25% 0.44-0.65% 415 MPa (60 ksi) 205 MPa (30 ksi)
P22 1.90-2.60% 0.87-1.13% 415 MPa (60 ksi) 205 MPa (30 ksi)
P91 8.00-9.50% 0.85-1.05% 585 MPa (85 ksi) 415 MPa (60 ksi)
P92 8.50-9.50% 0.30-0.60% 620 MPa (90 ksi) 440 MPa (64 ksi)

Minimum elongation, hardness, grain size and flattening requirements are tabulated by grade and wall thickness in the specification. Pipe is normally supplied with a hydrostatic test, and a nondestructive electric test may be substituted where agreed between purchaser and manufacturer.

Cross-Standard Equivalents

Buyers working to European or Japanese project specifications regularly need a mapping between ASTM A335 and the local standard. The closest families are EN 10216-2 for seamless steel tubes for pressure purposes, in which grades such as 13CrMo4-5 and 10CrMo9-10 sit alongside the 1.25% Cr and 2.25% Cr A335 types; JIS G3462, which covers STPA22, STPA23, STPA24 and similar boiler and heat-exchanger tube grades; and GB/T 5310, the Chinese standard for seamless steel tubes for high-pressure boilers, which includes grades such as 15CrMoG and 12Cr2MoG. The correspondence is approximate because allowable stresses, tolerances and testing regimes differ between standards, so the design code always governs.

Applications and Selection Points

Typical duties include superheater and reheater tubing, main steam and hot reheat piping, boiler headers, hydrogen and hydrotreating process lines, reformer furnace tubes and high-temperature transfer lines. When selecting a grade, the first question is the design metal temperature: the allowable stress tables of ASME B31.1 or ASME B31.3 fall steeply once the material enters the creep range, and that is what decides whether a 1.25% Cr, 2.25% Cr or 9% Cr grade is required. Wall thickness, thermal fatigue from cycling, oxidation and steam-side scaling are the other controlling factors. Welding a chromium-molybdenum pipe requires qualified procedures, consumables matched to the grade family and, for most grades and wall thicknesses, post-weld heat treatment at a temperature set by the governing code. Pipe for these services should also be checked for hardness and, on the 9% Cr grades, for a fully martensitic microstructure after heat treatment.

FAQ

Q: What is the difference between ASTM A335 P11 and P22?
The difference is mainly chromium content: P11 contains 1.00 to 1.50% Cr while P22 contains 1.90 to 2.60% Cr, both with about 1% Mo. P22 therefore has higher creep strength at temperature and is used for hotter sections, while P11 suits moderately elevated temperature duty.

Q: Is ASTM A335 pipe always seamless?
Yes. The specification covers seamless ferritic alloy-steel pipe only, so welded pipe cannot be certified as ASTM A335, although equivalent welded products are covered by other ASTM specifications for high-temperature service.

Q: How hot can ASTM A335 grades be used?
The upper limit is set by the allowable stress tables of the applicable design code rather than by the material specification alone. Chromium-molybdenum grades are used well into the creep range, and the 9% Cr grades extend service to higher steam temperatures than the 1.25% and 2.25% Cr types.

Q: What testing is carried out on A335 pipe?
Heat and product chemical analysis, tensile testing, hardness checks, dimensional inspection, a hydrostatic test or an approved nondestructive electric test, plus visual and, when specified, ultrasonic inspection of the wall.

Q: Does A335 pipe have to be post-weld heat treated?
For most grades and section thicknesses the governing code requires post-weld heat treatment to temper the weld and heat-affected zone and restore creep properties. The code also allows exemptions for thin sections, so the requirement should always be read against the specific grade, thickness and service.

Send Inquiry