What Is EN 10297-1 20NiCrMo2-2?
20NiCrMo2-2, steel number 1.6523, is a nickel-chromium-molybdenum case-hardening steel supplied as seamless tube under EN 10297-1. The designation follows the European case-hardening steel convention: the leading figure gives the nominal carbon content in hundredths of a percent, followed by the alloying elements and their nominal content.
Tubes made from this grade are used where a hard, wear-resistant surface must be combined with a tough, shock-resistant core. The low carbon content keeps the core ductile after quenching, while the nickel, chromium and molybdenum additions provide the hardenability needed for the carburised case to develop an effective depth of hardness.
Chemical Composition and Alloy Design
| Element | Content % | Contribution |
|---|---|---|
| Carbon | 0.17 to 0.23 | Core strength after hardening, case response |
| Silicon | 0.40 max | Deoxidation |
| Manganese | 0.60 to 0.90 | Hardenability, sulphur control |
| Phosphorus | 0.025 max | Residual, capped for toughness |
| Sulphur | 0.035 max, lower for improved grades | Residual, controlled for machinability balance |
| Chromium | 0.40 to 0.60 | Hardenability and case carburising response |
| Nickel | 0.40 to 0.70 | Toughness, especially at low temperature |
| Molybdenum | 0.15 to 0.25 | Resistance to temper embrittlement |
The composition is deliberately balanced rather than highly alloyed. Nickel improves the low-temperature toughness of the core, chromium and manganese build the hardenability required for the case, and molybdenum suppresses temper embrittlement during the tempering step that follows quenching. Residual elements are held low so that the tube remains clean and predictable in service.
Mechanical Properties and Hardness
Properties depend on the heat treatment route and on the wall thickness of the tube, because hardenability is limited by section size. The two conditions normally quoted are the normalized or annealed delivery condition, in which the tube is soft and readily machined, and the quenched and tempered condition, in which the tube reaches its working strength.
| Condition | Typical outcome |
|---|---|
| Soft annealed or normalized delivery condition | Machinable structure for forming, turning and cutting |
| Quenched and tempered | High tensile and proof strength with good notch toughness |
| Carburised and hardened case | Case hardness in the region of 58 to 62 HRC with a controlled case depth |
| Core after carburising and hardening | Tough core, hardness dependent on section size and hardenability |
Because hardenability is moderate, the achievable core hardness falls as wall thickness increases, and properties are therefore specified against the wall thickness band rather than as a single figure. Where the design relies on core strength, the tube wall and the quench severity must be matched to the hardenability of the steel. Where the design relies on wear resistance, the case depth and case hardness are the controlling values, and these are agreed with the heat treater for the specific tube size.
Heat Treatment Cycle
Austenitising in the range of about 830 to 860 degrees Celsius, followed by oil quenching to convert the structure to martensite.
Tempering in the range of about 550 to 600 degrees Celsius to balance strength and toughness. Raising the tempering temperature increases toughness and reduces strength.
Optional case hardening by carburising in the range of about 900 to 930 degrees Celsius followed by quenching, to produce a hard case over a tough core.
No slow cooling through the temper embrittlement range after tempering, to preserve notch toughness.
The tempered structure is tempered martensite with finely dispersed alloy carbides. Control of the austenitising temperature and time is important because an unnecessarily coarse prior austenite grain size reduces toughness in the finished part.
Typical Applications
Aerospace shafting and structural tubular components subject to fatigue loading
Automotive drivetrain parts such as gear shafts and high stress rotating components
Energy industry components requiring toughness at sub-zero ambient temperature
Machine tool spindles, sleeves and bushes needing a hard wearing surface
Hydraulic and pneumatic actuator components where a hard bore or rod surface is required
General precision mechanical parts produced from tube stock on automatic machines
Testing and Traceability
Inspection of EN 10297-1 tube normally covers dimensional verification of outside diameter and wall thickness, chemical analysis per cast, tensile testing per batch, and hardness testing where the order requires it. Ultrasonic testing is used for internal soundness and magnetic particle or dye penetrant inspection for surface defects on tube intended for fatigue-critical components.
Metallurgical checks may include prior austenite grain size determination and non-metallic inclusion rating when the application demands clean steel. Material certification is issued to the inspection level agreed in the order, with full traceability from the cast number to the finished tube, and any supplementary requirements such as a specific surface finish or end preparation are stated in the purchase specification.
FAQ
Q: What does the designation 20NiCrMo2-2 mean?
The leading figure 20 indicates approximately 0.20 percent carbon, the letters identify nickel, chromium and molybdenum as the alloying elements, and the final figures indicate their nominal content, giving steel number 1.6523.
Q: Is this grade meant for surface hardening or through hardening?
It is a case-hardening steel. Components are normally carburised and hardened to obtain a hard, wear-resistant surface over a tough core, although the tube can also be quenched and tempered for through strength.
Q: What case hardness can be expected?
A correctly carburised and hardened case typically reaches the region of 58 to 62 HRC, while the core hardness depends on the wall thickness and the hardenability of the steel.
Q: Why is molybdenum included in the composition?
Molybdenum improves hardenability and, more importantly, resists temper embrittlement so that notch toughness is retained after tempering.
Q: What is the recommended heat treatment temperature range?
Austenitising is carried out around 830 to 860 degrees Celsius followed by oil quenching, with tempering in the region of 550 to 600 degrees Celsius, and carburising around 900 to 930 degrees Celsius when case hardening is required.
Q: How is the tube inspected?
Inspection covers dimensional checks, chemical analysis, tensile testing and hardness testing, supplemented by ultrasonic and surface defect examination for fatigue-critical applications, all with traceability to the cast number.