What A671 CC60 Is
ASTM A671, with its ASME twin SA-671, is the standard for electric-fusion-welded (EFW) carbon steel pipe for atmospheric and lower-temperature service. In CC60, the letters CC identify the base plate specification, ASTM A537 Class 1, and the number 60 is the minimum tensile strength of the finished pipe in ksi, equal to about 415 MPa. The pipe is formed from plate and the longitudinal seam is welded by automatic submerged arc welding, and it serves large-diameter piping in refineries, power stations, chemical plants, and refrigerated facilities where seamless pipe of the required size is not available.
The Class Number: Heat Treatment, Not Pressure
The class number in the A671 designation defines the heat treatment of the finished welded pipe. The valid classes are 10, 20, 30, 40, 50, 60, 70, and 80: Class 10 is supplied without post-weld heat treatment, and the higher classes add stress relief, normalizing, normalizing and tempering, or quenching and tempering. Class numbers such as 32 are not defined in the standard, and the class is not a pressure rating. The allowable pressure of the pipe is calculated from the wall thickness, the diameter, the grade, and the design code; descriptions that attach a pressure rating to a class number do not reflect the standard.
| Class | Heat treatment |
|---|---|
| 10 | No post-weld heat treatment |
| 20 / 30 | Stress relief / normalizing |
| 40 | Normalizing and tempering |
| 50 – 80 | Quenching and tempering variants |
Material and Properties
The base plate, A537 Class 1, is a killed, fine-grain carbon steel with a minimum yield strength of 50 ksi (345 MPa) for plate up to 2.5 inches and a tensile range of 70 to 90 ksi. Typical composition limits are about 0.24% carbon maximum, 0.70 to 1.60% manganese, 0.035% phosphorus, and 0.035% sulphur. The finished pipe, tested per A671, must meet the tensile and bend requirements of the standard, and for lower-temperature service it is Charpy impact tested at the design temperature.
Testing and Certification
A671 requires tensile testing of the base metal and the weld, guided bend tests of the weld, hydrostatic testing, and non-destructive examination of the longitudinal weld, normally by radiography, with the extent agreed for the service. The mill certificate, to EN 10204 3.1 or 3.2, states the standard and edition, the grade, the class, the plate specification, the chemistry, the mechanical results, the heat-treatment details, and the NDE results. The certificate is the controlling document for verifying the delivered product against the order.
Service Scope and Limits
A671 pipe is used for atmospheric and lower-temperature service down to about -50 F (-45 C) for impact-tested grades. It is not designed for extreme-pressure service: the high-pressure EFW product for moderate temperatures is covered by A672, and alloy or cryogenic service is covered by other specifications. A description that promises pressures far above the design-code values of a 60 ksi tensile pipe, or service at cryogenic temperatures, is inconsistent with the standard and should be rejected at the specification stage.
Verifying the Specification
Before ordering, verify every element of the description against the current edition of the standard: the grade letters and the strength number, the class number from the valid list, and the pressure and temperature claims derived from the design code. Require the mill certificate to state the exact designation. This discipline keeps fabricated specifications, which have circulated in the market, out of the supply chain.
Frequently Asked Questions
Q: What does CC60 mean in A671?
The letters CC identify the base plate per ASTM A537 Class 1, and 60 is the minimum tensile strength of the finished pipe in ksi, about 415 MPa.
Q: What classes does A671 define?
Classes 10 to 80 in steps of ten, describing the heat treatment of the finished pipe. Class numbers such as 32 are not part of the standard.
Q: Is the class a pressure rating?
No. The class defines the heat treatment; the pressure rating comes from the dimensions and the design code.
Q: What is the low-temperature limit of A671?
Impact-tested grades cover service down to about -50 F (-45 C). Colder cryogenic service requires materials such as A333 or austenitic stainless steel.
Q: What tests are required?
Tensile, guided bend, hydrostatic, and non-destructive tests of the weld, with Charpy impact testing for lower-temperature service.
Q: How is the specification verified?
By checking the grade, strength number, and class against the standard, and requiring the mill certificate to state the exact designation and test results.