ASTM A335 P22 Seamless Alloy Steel Pipe for High-Temperature Service
ASTM A335 P22 is a widely used specification for seamless ferritic alloy-steel pipe designed for high-temperature and high-pressure service. The "P" designates it for Pressure Piping systems. Its common name is 2¼ Chromium - 1 Molybdenum (2¼Cr-1Mo) steel.
Key Characteristics
| Feature | Description |
|---|---|
| Material Type | Ferritic Alloy Steel (Chromium-Molybdenum) |
| Manufacturing | Seamless (SMLS) only |
| Common Names | 2¼Cr-1Mo, Grade 22, WP22 |
| Key Property | Excellent creep strength and oxidation resistance at elevated temperatures (up to ~593°C / 1100°F) |
| Primary Use | High-temperature piping in power plants, refineries, and petrochemical facilities (e.g., steam lines, headers, process piping) |
Chemical Composition (Ladle Analysis)
| Element | Composition (%) |
|---|---|
| Carbon (C) | 0.05 – 0.15 |
| Manganese (Mn) | 0.30 – 0.60 |
| Phosphorus (P), max | 0.025 |
| Sulfur (S), max | 0.025 |
| Silicon (Si), max | 0.50 |
| Chromium (Cr) | 1.90 – 2.60 |
| Molybdenum (Mo) | 0.87 – 1.13 |
Mechanical Properties
Condition: Normalized & Tempered
| Property | Requirement |
|---|---|
| Tensile Strength, min | 415 MPa (60,000 psi) |
| Yield Strength, min | 205 MPa (30,000 psi) |
| Elongation (in 50mm), min | 30% |
| Hardness, max | 250 HBW / 265 HV |
Heat Treatment & Metallurgy
Mandatory Heat Treatment: P22 pipe must be supplied in the fully annealed, or normalized and tempered condition.
Purpose: This refines the grain structure, ensures uniform properties, and achieves the required toughness and strength.
Post-Weld Heat Treatment (PWHT): Required for most welding to prevent cold cracking and relieve stresses. Typical range: 677°C – 746°C (1250°F – 1375°F).
Common Applications
Power Generation: Main steam lines, hot reheat lines, headers, and other high-energy piping.
Refineries: Fluid Catalytic Cracking (FCC) units, hydrocracker units, and other high-temperature process lines.
Petrochemical: High-temperature transfer lines and process piping.
Comparison with Related Grades
| Grade | Key Difference from P22 |
|---|---|
| P11 (1¼Cr-½Mo) | Lower chromium & molybdenum. Lower high-temperature strength. |
| P5 (5Cr-½Mo) | Higher chromium, better oxidation resistance but different strength profile. |
| P9 (9Cr-1Mo) | Higher chromium, significantly better oxidation resistance. |
| P91 (9Cr-1Mo-V) | Modern grade with vanadium/niobium for much higher creep strength. |
| A106 Gr. B | Carbon steel. Not suitable for high-temperature service (>~425°C). |
Important Notes for Users
T22 vs. P22: ASTM A213 T22 is the equivalent material for tubes (used in boilers, superheaters). They share identical chemistry but differ in product form and application (tube vs. pipe).
Temperature Limit: P22 is typically used for service up to 593°C (1100°F). For higher temperatures, grades like P91 are preferred.
Welding: Requires careful welding procedures with matching or over-matching filler metals (e.g., AWS ER90S-B3, E9015-B3) followed by mandatory PWHT.
Corrosion: Offers good resistance to hydrogen attack and sulfide corrosion at elevated temperatures, making it suitable for refinery service.
In summary, ASTM A335 P22 is a workhorse alloy steel for critical high-temperature piping, offering a reliable balance of strength, fabricability, and cost for demanding industrial applications.